Restoration of Obliterated Stamped Marks on Aluminium Surfaces by Metallographic Etching Technique
Amit Kumar, Ankit Srivastava, Tanurup Das, Abhimanyu Harshey, Veer Raj Saini, Akash Kumar, Md. Alim, Kriti Nigam and Vijay Kumar Yadav
Department of Forensic Science and Criminology, A.P.J. Abdul Kalam Institute Bundelkhand University, Jhansi 284128, Uttar Pradesh, India.
Corresponding Author E-mail: vijayforensic01@gmail.com
DOI : http://dx.doi.org/10.13005/ojc/360628
Article Received on : 11-11-2020
Article Accepted on : 13-12-2020
Article Published : 31 Dec 2020
Serial number restoration is a frequently encountered problem in forensic science laboratories for the investigation of theft and burglary cases. These identification marks are generally introduced over metallic surfaces of different vehicle parts and firearms by various means. Chemical etching is one of the most effective and simple technique to restore obliterated, erased, over-stamped, and over-engraved marks on metallic surfaces. Several significant studies on restoration of engraved markings on aluminium surfaces were previously reported. The present study attempts to find out an efficient and fast etching reagent to restore obliterated stamped marks on aluminium surfaces. Ten effective etching reagents previously reported by various researchers in their restoration studies were assessed in the present experiment. Etching reagents were individually applied on obliterated surfaces by the cotton swabbing method. The Reagent 3 (ferric chloride 25 g, conc. HCl 25 ml, distilled water 100 ml) was found out to be the most sensitive and rapid (4 – 6 minutes) for the restoration on aluminium surfaces. The study also revealed that the absence of an alkaline compound in etching reagent potentially accelerates the speed of the restoration process.
KEYWORDS:Aluminium; Etching Reagent; Obliteration; Restoration; Stamped Marks; Serial Number
Download this article as:Copy the following to cite this article: Kumar A, Srivastava A, Das T, Harshey A, Saini R. V, Kumar A, Alim M, Nigam K, Yadav K. V. Restoration of Obliterated Stamped Marks on Aluminium Surfaces by Metallographic Etching Technique. Orient J Chem 2020;36(6). |
Copy the following to cite this URL: Kumar A, Srivastava A, Das T, Harshey A, Saini R. V, Kumar A, Alim M, Nigam K, Yadav K. V. Restoration of Obliterated Stamped Marks on Aluminium Surfaces by Metallographic Etching Technique. Orient J Chem 2020;36(6). Available from: https://bit.ly/2WYnuJQ |
Introduction
Serial numbers are unique identification marks placed on engines and chassis of vehicles, firearm frames or any other metallic object1 – 4. Casting, Engraving, die stamping, pin stamping and LASER are commonly used to introduce these identification marks on the metallic surfaces 5,6. On the contrary, perpetrators frequently obliterate or remove these marksby several mechanical means i.e., peening, punching, filing, grinding, drilling, welding over-stamping, chemical corrosion, etc.for unauthorized selling and to avoid any connection with the item1, 2, 6 – 8. Restoration of the obliterated or removed identification marks provides major leads in the identification of stolen objects2,9. The marking process deforms several layers underneath the actual indentation. The depth of deformation depends on the strength of the metal, i.e., on impact, zinc deforms more than iron10 (Figure 1.a – 1.c). The efficiency of restoration depends upon the depth of obliteration. Treatment of the surface with different chemicals known as macro etching is the most common restoration technique used by the researchers on metals. Macro etching is the most effective metallographic technique among all11.
Figure 1: Cross – sectional of deformed crystal structure by mechanical force. |
A desirable etching reagent for metallic surfacealways give good contrast, reproducibility and consume less time for restoration. A large number of significant studies have been performed on commonly encountered metals and their alloys. Works by Turley12, Zaili et al.7, Wightman and Matthew1, yin and Kuppuswamy13, Wahab et al.11 and Richa et al.4, showed that different composition of ‘Fry’s Reagent’ consists of a metallic halide or salts and a strong acid is an excellent etching reagent for iron and steel surfaces. Recently Shankar et al.3 restored obliterated serial markings on copper by a combination of ferric chloride, glacial acetic acid and distilled water and Fortini et al.14restored obliterated markings on Ni-Cr-Mo steel surface by a combination of Nitric acid and distilled water.
Aluminium and its alloys are rapidly replacing other metals in the vehicle, firearm and machinery industry in recent decades due to its strength and lightweight2,15-16. Different alloys (e.g. Duralumin) of aluminium also used frequently in various automobile industries16.Restoration on aluminium surfaces were previously performed only on obliterated engraved marks2,9,10,15,17. Studies by Chisum15, Baharumet al.10, Peeler et al.17 Bong and Kuppuswamy9 and Uli et al.2 revealed that etching reagents used for comparatively strong metals and their alloys like iron, steel, etc. are not suitable for the restoration of obliterated engraved marks on aluminium and its alloy surfaces. Few researchers recommended that an alternate application of a dilute solution of a strong acid and a strong alkali can be a good etching reagent on aluminium surfaces2,9-10. Present study assessed ten best etching reagents used in previous studies of restoration on different metallic surfaces to find out a fast and effective reagent for the restoration of obliterated stamped marks on aluminium surface.
Methodology
In the present study 12.1 mm thick aluminium bricks were used to restore obliterated serial numbers created by punching method. Metallographic etching or chemical etching techniques is used for the restoration in the present study. The procedure of this method has been adapted from the previous studies of restoration of obliterated engraved marks on aluminium and it alloy surfaces2,9,10,15,17
Sample Preparation
A stamping die was used to introduce numeric characters from 1 to 9. Each character of the die stamp covers approximately 0.3 square inch area. Finally, all the samples were obliterated by the mechanical grinding machine (Figure 2) up to zero visibility. Samples were photographed before and after each step for permanent record and comparison.
Figure 2: Grinder used to create the obliteration on aluminium surface |
Preliminary Examination and Surface Preparation
Surface preparation before restoration is the compulsory step as it makes the surface uniform which in turn enhance the efficiency of the restoration. All the samples were first examined by a magnifying lens to observe any remaining visible number. Commercially available silicon carbide paper (P60) is used to polish the grinded surface by removing scratches and other marks to give a smooth mirror-like finish for better chemical treatment. Polishing is followed by swabbing the surface with acetone to remove any dirt, grease, paint or any other loosely adherent material from the surface.
Chemical Etching
In the present work ten etching reagents (Table 1) were selected from previous studies of restoration on metallic surfaces. All the selected reagents are best in their respective studies. Reagent 1, 2 and 6 were previously used on the aluminium and its alloy surfaces (Al-Zn-Mg-Cu and Al-Si). Reagents were applied on the obliterated surface by swabbing method. A cotton bud is soaked in the reagent and gently applied over the obliterated aluminium surfaces until the marks restored. Single reagents were swabbed uninterruptedly and multi-reagents were applied alternatively until the numbers restore. Since, the restored numbers were visible for a short period of time,instant photographs were captured to keep a permanent record before and after every step. The application method and composition of each reagent are summarized in the Table 1.
Table 1: Comparative effectiveness and sources of chemical etching reagents for the restoration of obliterated stamped marks on aluminium surfaces.
S. No. |
Etching Reagent |
Composition of Reagent |
Application Method |
Consumed Time |
Observation |
Source |
1. |
Reagent 1 (Villella’s reagent) |
Glycerine 30 ml Hydrofluoric acid 20 ml Nitric acid 10 ml |
Continuously swabs the reagent until the numbers appear. |
20 – 25 |
Both contrast and reproducibility were good and can be easily photographed. |
Heard, 2008 |
2. |
Reagent 2 (Hume Rothery solution) |
Copper Chloride (CuCl2) 200 g Hydrochloric Acid (HCl) 5 ml Distilled water 1000 ml |
The solution was swabbed alternatively on the erased surface. First with Hume Rothery solution and then with distilled water. |
20 |
The number appears in good contrast and also reproducible. |
Baharum et al., 2008, Heard, 2008 |
3. |
Reagent 3 |
Ferric Chloride (FeCl3) 25 g HCl 25 ml Distilled water 100 ml |
The reagent was swabbed continuously until the numbers appear. |
4 – 6 |
Good contrast, easily observed and reproducible. Can be easily photographed. |
Richa et al., 2012 |
4. |
Reagent 4 |
Solution 1 Copper Chloride 45 g HCl 100 ml Distilled water 180 ml
Solution 2 15% Nitric acid |
Both solutions were swabbed alternatively on the erased surface. until the numbers appear. |
90 |
No restoration. |
Wahab et. al., 2012 |
5. |
Reagent 5 |
Conc. HCl 10 ml Glacial acetic acid 25 ml |
The solution was applied continuously until the numbers appear. |
30 |
Numbers appeared in fair contrast and slightly observable and also reproducible. |
Shankar et al., 2014 |
6. |
Reagent 6 |
Solution 1 10% Sodium hydroxide
Solution 2 10% Nitric acid |
Both the solution was swabbed alternatively on the erased surface. First with solution 1 for 3 minutes. Then solution 2 for 1 minute. |
60 |
Both contrast and reproducibility were good and the sensitivity of numbers was also good. |
Uli et al. 2010, Petterd, 2000 Bong and Kuppuswamy, 2010 |
7. |
Reagent 7 |
Solution 1 10% Sodium hydroxide (NaOH)
Solution 2 25% Nitric acid (HNO3) (Used as highlighter for the above chemical) |
Swabs with NaOH and then HNO3 |
58 |
Technical Procedure of reagent preparation 2014 |
|
8. |
Reagent 8 |
10% Sodium hydroxide Distilled water 90 ml |
Continuusly swabbing over the erased surface until the numbers appear. |
50 |
Numbers are reproducible and appeared in good contrast. |
Katterwe, 2006 |
9. |
Reagent 9 |
Nitric acid 25 ml Distilled water 75 ml |
90 |
No restoration. |
Petterd, 2000 |
|
10. |
Reagent 10 |
Nitric acid 20 ml Potassium permanganet 4 g Distilled water 100 ml |
90 |
Shankar et al., 2014 |
Results
The present study is focused to find out an effective and rapid chemical reagent to restore obliterated stamped serial numbers on aluminium surfaces. Several researchers explored multiple reagents to restore obliterated serial numbers on different metallic surfaces. 10 best etching reagents from different restoration studies on aluminium and other metallic surfaces were selected for the present experiment. The experimental result shows that 7 among 10 reagents (i.e., Reagent 1: Glycerine 30 ml, Hydrofluoric acid 20 ml, Nitric acid (HNO3) 10 ml, Reagent 2: Copper Chloride 200 g, Hydrochloric Acid 50 ml, Distilled water 1000 ml, Reagent 3: Ferric Chloride 25 g, Hydrochloric Acid 25 ml, Distilled water 100 ml, Reagent 5: Conc. Hydrochloric Acid 10 ml, Glacial acetic acid 25 ml, Reagent 6: 10% Sodium hydroxide (NaOH), 10% HNO3, Reagent 7: 10% NaOH, 25% HNO3 and Reagent 8: 10% NaOH, Distilled water 90 ml.) successfully restored the obliterated marks. But, only three reagents i.e., Reagent 1 (Villella’s reagent), Reagent 2 (Hume Rothary Solution) and Reagent 3 (Ferric Chloride 25 g, Hydrochloric Acid 25 ml, Distilled water 100 ml) showed good restoration efficiency in less time (4-25 min) Figure 3.a-3c, 4a-4.c). Reagent 3 was the standout among all as it took the least time (4 – 6 Minutes) and also produce good visibility (Figure 5.a – 5c) of restored numbers. This experiment also revealed that reagents containing alkali, took comparatively less time (4 – 30 minutes) to restore the obliterated marks than the reagents containing it (50 – 60 minutes). Table 2 shows the comparative representation of the consumed time by reagents including alkali and without alkali. Reagent 4, 9 and 10 showed no restoration on the aluminium surface.
Figure 3: Serial mark(a) pre obliteration (b) post obliteration (c) restored by Villella’s Reagent |
Figure 4: Serial mark(a) pre obliteration (b) post obliteration (c) restored by Hume Rothary solution |
Figure 5: Serial mark (a) pre obliteration (b) post obliteration (c) restored by Reagent 3 |
Table 2: The comparative representation of the consumed time by reagents including alkali and without alkali.
Reagent (Without Alkali) |
Composition |
Consumed Time (Min) |
Reagent (Including Alkali) |
Composition |
Consumed Time (Min) |
Reagent 1 (Villella’s reagent) |
Glycerine 30 ml Hydrofluoric acid 20 ml Nitric acid(HNO3) 10 ml |
20 – 25 |
Reagent 6 |
Solution 1 10% Sodium hydroxide
Solution 2 10% Nitric acid |
60 |
Reagent 2 (Hume Rothery solution) |
Copper Chloride (CuCl2) 200 g Hydrochloric Acid (HCl) 5 ml Distilled water 1000 ml |
20 |
Reagent 7 |
Solution 1 10% Sodium hydroxide (NaOH)
Solution 2 25% Nitric acid (HNO3) (Used as highlighter for the above chemical) |
58 |
Reagent 3 (Fry’s Reagent) |
Ferric Chloride (FeCl3) 25 g HCl 25 ml Distilled water 100 ml |
4 – 6 |
Reagent 8 |
10% Sodium hydroxide Distilled water 90 ml |
50 |
Reagent 5 |
Conc. HCl 10 ml
Glacial acetic acid 25 ml |
30 |
|
Discussion
Richaet al.4 performed a similar experiment on steel surface by using multiple combinations of Fry’s reagent and found effective results. Reagent3 produced the best visibility in minimum time (4 – 6 min.) with better reproducibility among all the ten reagents used. In the study by Chisum15, a similar combination of metallic chloride (Mercuric Chloride) and a strong acid (HCl) showed good restoration on aluminium and its alloy surfaces that is similar with the results of the present study. An alternative swabbing of 60% Hydrochloric Acid (HCl) and 40% NaOHproved to be a good etching reagent for obliterated engraved marks on aluminium and its alloys in the experiments by Baharum et al.,10 Bong and Kuppuswamy9 and Peeler et al.,17. Uli et al. used an alternate swabbing of 10% Nitric Acid and 10% NaOHin their study which showed good results on aluminium-silicon alloy surfaces2. Previous studies revealed that the effect of etching reagent on the metal surface is affected by the marking procedure. Engraved aluminium surfaces did not restore obliterated marks by the etching reagents used for strong metals because it corrodes most of the underlying shallow deformations2,9-10. Stamping method potentially causes greater deformation on the metal surface that make it persistentto the exposure of strong etching reagents as observed in the present study (Reagent 3). Previous studies suggested that aluminium and its alloys show gradual corrosion to the exposure of caustic solutions like an alkali2. NaOH(Alkali) is present in most of the best-suited reagents previously used for aluminium and its alloys2,9,17. The absence of alkali probably accelerates the caustic effect on the aluminium surface that reduces the restoration time. The reagents without NaOH (i.e., Reagent 2, 3 and 5) restored the obliterated serial numbers faster than the reagents consisting NaOH.A comparison between the results of the previous and the present study on aluminium surfaces is summarized in Table 3.
Table 3: Summarized table of previous and present study on aluminium surfaces.
Comparative Study |
|||
S.No. |
Study |
Composition Of Desirable Reagent |
Restoration Time (Minutes) |
1. |
Chisum WJ, 1963 |
0.1M Mercuric Chloride in 0.1N Hydrochloric Acid |
20 |
2. |
Baharumet al. 2008 |
Solution 1 60% hydrochloric acid Solution 2 40% sodium hydroxide |
3 – 60 |
3. |
Uliet al. 2010 |
Solution 1 10% Sodium hydroxide Solution 2 10% Nitric acid |
8 – 40 |
4. |
Bong and Kuppuswamy, 2010 |
(i) 10% Aqueous Phosphoric Acid (ii) Solution 1 60% hydrochloric acid Solution 2 40% sodium hydroxide |
2 – 960
2 – 20 |
5. |
Present Study |
Ferric Chloride 25 g Hydrochloric acid 25 ml Distilled water 100 ml |
4 – 6 |
Conclusion
The present study is the first attempt to restore obliterated stamped serial numbers on the aluminium surface in contrast to all the previous studies on obliterated engraved markings.Among 10 chemical reagents used, reagent 3 (Ferric Chloride 25 g, HCl 25 ml and Distilled water 100 ml) produce desired results in minimum time (4 -6 min). The study also revealed that the absence of the alkaline compound potentially enhances the caustic effect to minimize the restoration time. Reagent 2, 3 and 5 including HCl showed a similar result as produced by reagent 6, 7 and 8 including NaOH. But acid-containing reagents took lesser time to restore the obliterated numbers.
References
- Wightman, G.; Matthew, J. Restoration of stamp marks on steel components. Forensic Science International.,2008, 180, 32–36. DOI: 10.1016/j.forsciint.2008.06.017.
CrossRef - Uli, N.;Kuppuswamy, R.;Amran, M.F.C. A survey of some metallographic etching reagents for restoration of erased engraved marks on aluminium–silicon alloy surfaces. Forensic science International.,2010, 208, 66-73. DOI: 10.1016/j.forsciint.2010.11.005.
CrossRef - Shankar, N.;Kesharwania, L.; Mishra, M.K.;Chattree, A.; Kumar, R.; Sharma, R.; Gupta.A.K.New Restoration Reagent for Development of Erased Serial Number on Copper Metal Surface. Malaysian Journal of Forensic Sciences.,2014, 5(2), 53-66.
- Richa.;Kesharwani, L.; Gupta, A.K.; Mishra, M.K. Development of new reagent for restoration of erased serial number on metal plate. Egyptian journal of Forensic Science.,2013, 3(1), 26-34. DOI: dx.doi.org/10.1016/j.ejfs.2012.11.004.
CrossRef - Nickols, L.C.The Scientific Investigation of Crime.London:Butterworth & Co., 1956.
CrossRef - Heard, B.J. Handbook of firearms and ballistics: Examining and interpreting forensic science evidence. 2nd ed.Hoboken NJ: Wiley John& Sons.,2008.
CrossRef - Zaili, M.A.M.;Kuppuswamy, R.;Harun, H. Restoration of engraved marks on steel surfaces by etching technique. Forensic science International.,2006, 171, 27-32. DOI: 10.1016/j.forsciint.2006.09.010.
CrossRef - Kuppuswamy, R.;Senthilkumar, M. Restoration of vehicle identification numbers. Journal of forensic Identification.,2004, 54, 13–21.
- Bong, Y.U.;Kuppuswamy, R. Revealing obliterated engraved marks on high strength aluminium alloy (AA7010) surfaces by etching technique. Forensic Science International.,2010, 195, 86–92. DOI: 10.1016/j.forsciint.2009.11.018.
CrossRef - Baharum, M.I.M.;Kuppuswamy, R.; Rahman, A.A. Recovering erased engraved marks on aluminium surfaces by etching technique. Forensic Science International.,2008, 177, 221-227. DOI: 10.1016/j.forsciint.2008.01.004.
CrossRef - Wahab, M.F.A.;Izwani, N.;Ghani.M.;Kuppuswamy, R. An investigation into the suitability of some etching reagents to restoring obliterated stamped numbers on cast iron engine blocks of cars. Forensic Science International.,2012, 223, 53–63.DOI:dx.doi.org/10.1016/ j.forsciint.2012. 07.02012.
CrossRef - Turley, D. Restoration of Stamp Marks on Steel Components by Etching and Magnetic Techniques. Journal of Forensic Sciences., 1987, 32(3), 640-649. DOI: doi.org/10.1520/JFS12368J13.
CrossRef - Yin, S.H.;Kuppuswamy, R. On the sensitivity of some common metallographic reagents to restoring obliterated marks on medium carbon (0.31% C) steel surfaces. Forensic Science International.2009, 183, 50–53. DOI: 10.1016/j.forsciint.2008.10.009.
CrossRef - Fortini, A.; Merlin, M.;Soffritti, C.;Garagnani, G.L. Restoration of Obliterated Numbers on 40NiCrMo4 Steel by Etching Method: Metallurgical and Statistical Approaches. Journal of Forensic Science.2016, 61(1), 160 – 69. DOI: 10.1111/1556-4029.12849.
CrossRef - Chisum, W.J. A catalytic process for restoration of serial numbers on aluminium. Journal of Forensic Science Society.,1966, 6(2), 89.
CrossRef - Okayasu, M.; Sato, K.; Mizuno, M. A new etching technique for revealing the plastic deformation zone in an Al–Cu–Mg alloy. Journal of Material Science.,2008, 43, 2792–98. DOI: 10.1007/s10853-008-2544-y.
CrossRef - Peeler, G.;Gutowski, S.;Wrobel, H.; Dower, G. The restoration of impressed characters on aluminium alloy motorcycle frames. Journal of Forensic Identification.2008, 58(1), 27–32.